ASTM A572 Grades
A572 Mechanical Requirements | ||||
---|---|---|---|---|
Grade | Yield, min ksi | Tensile, min ksi | Elongation, min % in 8” | Elongation, min % in 2” |
50 | 50 | 65 | 18 | 21 |
55 | 55 | 70 | 17 | 20 |
60 | 60 | 75 | 16 | 18 |
65 | 65 | 80 | 15 | 17 |
A572 Chemical Requirements | ||||||
---|---|---|---|---|---|---|
Alloy Group | Maximum Diameter, inches | Carbon, max% | Manganese, max% | Phosphorus, max% | Sulfur, max% | Silicon, max% |
50 | 4 | 0.23 | 1.35 | 0.04 | 0.05 | 0.4 |
55 | 2 | 0.25 | 1.35 | 0.04 | 0.05 | 0.4 |
60 | 1/1/2004 | 0.26 | 1.35 | 0.04 | 0.05 | 0.4 |
65 | 1/2 to 1-1/4 | 0.23 | 1.65 | 0.04 | 0.05 | 0.4 |
65 | Below 1/1 | 0.26 | 1.35 | 0.04 | 0.05 | 0.4 |
This abridged table shows only the chemical requirements for bars. The complete table including shapes and plates can be found in the ASTM standard at www.astm.org
In addition to the chemical requirements above, the material shall also contain enough alloying elements to meet the requirements of one of the below alloy types.
Alloy Content | ||
---|---|---|
Type | Elements | Heat Analysis, % |
1 | Columbium | 0.005 – 0.05 |
2 | Vanadium | 0.01 – 0.15 |
3 | Columbium | 0.005 – 0.05 |
Vanadium | 0.01 – 0.15 | |
Columbium plus Vanadium | 0.02 – 0.15 | |
5 | Titanium | 0.006 – 0.04 |
Nitrogen | 0.003 – 0.015 | |
Vanadium | 0.06 max |
All information derived from globally recognized specifications, subject to change, user discretion is advised.